September 12, 2014

Procedures

New Exfoliated Clay Film Synthesis

  1. Determine how much 4% exfoliated NaMT needed for 10% clay solution
    • 0.11 g=(Mass of 4% NaMT soln needed)*0.04
    • Mass of 4% NaMT soln needed=2.75 g
    • 2.7613 g 4% NaMT added
  2. Add ~1g PVA
    • 1.004 g PVA added
  3. Add 7 mL H2O
  4. Stir the solution with constant heating at 75C

Powder X-ray Diffraction Measurements

  • Sample prep:
    • Pat dry film soaked in 8 ppm malachite green solution
      • 200 ppm done by Andrew's group
      • 80 ppm done by Eleni's group
      • 2 ppm, plain PVA film, & NaMT powder done by James' group
    • Place film on pXRD disk
    • Press tape over film to hold in place, using a razor to cut off excess

Stock Solution Preparation

  • Make 200mL 200ppm
    • 40 mg MG in 200 mL volumetric flask
  • 80 ppm made by Eleni's group
  • 8 ppm made by Andrew's group
  • 2 ppm made by James' group

Soaking Films in Malachite Green Solutions

Note: all PVA films<br.>

  • 200 ppm
    • Vial mass: 13.1537 g
    • Vial + film mass: 13.2537 g
    • Film mass: 0.100 g
  • 2 ppm
    • Vial mass: 13.0783 g
    • Vial + film mass: 13.1843 g
    • Film mass: 0.106 g
  • 80 ppm
    • Vial mass: 13.0332 g
    • Vial + film mass: 13.1408 g
    • Film mass: 0.1076 g
  • 8 ppm
    • Vial mass: 13.0325 g
    • Vial + film mass: 13.1298 g
    • Film mass: 0.0973 g
  • Extra 10 mL 200 ppm and 10 mL 80 ppm with no PVA film put into glass vial to determine glass absorption of Malachite Green
  • Other groups extra solutions: