User:Megan L. Channell/Notebook/3D printing scaffolds with Au nanofibers/2014/02/18

From OpenWetWare
Jump to navigationJump to search
Project name Main project page
Previous entry      Next entry

Entry title

  • Make polydopamine for nanofibers
  • Myoglobin for procedure

Procedure

  • Preparing scaffolds
    • Immerse 4 PLA scaffolds (in 5mL test tube) in ~5mL of 10mM, pH 8.5 TRIS polydopamine solution for 1 hour
      • First two scaffolds immersed in solution pH 8.51
      • Second two scaffolds immersed in solution pH 8.59
    • Add 1mL 0.0621mM myoglobin to solution, shake test tube to combine solutions, allow surface functionalization to occur for 5 hours
    • Rinse with deionized water and allow scaffold to dry overnight

Results

  • Brute force
  • Scaffolds after 1 hr in Tris-polydopamine

  • Scaffolds after 5 hrs in Tris-polydopamine and Myoglobin solution