* Crosslink films made on [[User:Melissa_Novy/Notebook/CHEM-581/2012/10/03|2012/10/03]].
 
* Crosslink films made on [[User:Melissa_Novy/Notebook/CHEM-581/2012/10/03|2012/10/03]].
  
==Notes==
+
==PVOH Film Crosslinking==
 +
* The three films that were prepared on [[User:Melissa_Novy/Notebook/CHEM-581/2012/10/03]] were crosslinked.
 +
* Please refer to [[User:Moira_M._Esson/Notebook/CHEM-581/2012/10/05|Moira Esson's entry]] for masses and volumes of crosslinking solutions used.
 +
* Note that the two crosslinking solutions are 1% HCl in water and 0.2 M NaHCO<sub>3</sub>.
 +
** There were no deviations from the standard crosslinking protocol.
 +
** About 0.5 g was cut from each film and then crosslinked.  The rest of the film were saved for other analyses.
 +
 
 +
==AAS Analysis==
 
* The AA was found to be clogged with gold particles, so all measurements made on 2012/10/05 must be redone after the AA is properly cleaned.
 
* The AA was found to be clogged with gold particles, so all measurements made on 2012/10/05 must be redone after the AA is properly cleaned.
 
<!-- ##### DO NOT edit below this line unless you know what you are doing. ##### -->
 
<!-- ##### DO NOT edit below this line unless you know what you are doing. ##### -->

Revision as of 13:34, 22 October 2012

<!-- sibboleth --><div id="lncal1" style="border:0px;"><div style="display:none;" id="id">lncal1</div><div style="display:none;" id="dtext"></div><div style="display:none;" id="page">User:Melissa Novy/Notebook/CHEM-581/2012/10/05</div><div style="display:none;" id="fmt">yyyy/MM/dd</div><div style="display:none;" id="css">OWWNB</div><div style="display:none;" id="month"></div><div style="display:none;" id="year"></div><div style="display:none;" id="readonly">Y</div></div>

BDLlogo 300.png <sitesearch>title=Search this Project</sitesearch>

Customize your entry pages <html><img src="/images/a/aa/Help.png" border="0" /></html>

Objectives

  • Test Cu+2 solutions with atomic absorption.
    • Generate a calibration curve from Cu+2 standards.
  • Crosslink films made on 2012/10/03.

PVOH Film Crosslinking

  • The three films that were prepared on User:Melissa_Novy/Notebook/CHEM-581/2012/10/03 were crosslinked.
  • Please refer to Moira Esson's entry for masses and volumes of crosslinking solutions used.
  • Note that the two crosslinking solutions are 1% HCl in water and 0.2 M NaHCO3.
    • There were no deviations from the standard crosslinking protocol.
    • About 0.5 g was cut from each film and then crosslinked. The rest of the film were saved for other analyses.

AAS Analysis

  • The AA was found to be clogged with gold particles, so all measurements made on 2012/10/05 must be redone after the AA is properly cleaned.