Difference between revisions of "User:Megan L. Channell/Notebook/Masters Research/2014/01/29"

From OpenWetWare
Jump to: navigation, search
(Entry title)
(fix raw html notebook nav)
 
Line 2: Line 2:
 
|-
 
|-
 
|style="background-color: #EEE"|[[Image:owwnotebook_icon.png|128px]]<span style="font-size:22px;"> Project name</span>
 
|style="background-color: #EEE"|[[Image:owwnotebook_icon.png|128px]]<span style="font-size:22px;"> Project name</span>
|style="background-color: #F2F2F2" align="center"|<html><img src="/images/9/94/Report.png" border="0" /></html> [[{{#sub:{{FULLPAGENAME}}|0|-11}}|Main project page]]<br />{{#if:{{#lnpreventry:{{FULLPAGENAME}}}}|<html><img src="/images/c/c3/Resultset_previous.png" border="0" /></html>[[{{#lnpreventry:{{FULLPAGENAME}}}}{{!}}Previous entry]]<html>&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;</html>}}{{#if:{{#lnnextentry:{{FULLPAGENAME}}}}|[[{{#lnnextentry:{{FULLPAGENAME}}}}{{!}}Next entry]]<html><img src="/images/5/5c/Resultset_next.png" border="0" /></html>}}
+
|style="background-color: #F2F2F2" align="center"|[[File:Report.png|frameless|link={{#sub:{{FULLPAGENAME}}|0|-11}}]][[{{#sub:{{FULLPAGENAME}}|0|-11}}|Main project page]]<br />{{#if:{{#lnpreventry:{{FULLPAGENAME}}}}|[[File:Resultset_previous.png|frameless|link={{#lnpreventry:{{FULLPAGENAME}}}}]][[{{#lnpreventry:{{FULLPAGENAME}}}}{{!}}Previous entry]]&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;}}{{#if:{{#lnnextentry:{{FULLPAGENAME}}}}|[[{{#lnnextentry:{{FULLPAGENAME}}}}{{!}}Next entry]][[File:Resultset_next.png|frameless|link={{#lnnextentry:{{FULLPAGENAME}}}}]]}}
 
|-
 
|-
 
| colspan="2"|
 
| colspan="2"|

Latest revision as of 22:41, 26 September 2017

Owwnotebook icon.png Project name Report.pngMain project page
Resultset previous.pngPrevious entry      Next entryResultset next.png

Entry title

  • IMade two sets of molds. One from nanofibers from last semester and the other being Au NP citrate.
  • For the nanofiber first the solution was centrifuged:
    • 0.1% 0.993 g PLA, 10 mL of dichloromethane, approx. 1 drop of the nanofibers.
    • 0.5% 0.9949 g PLA, 10 mL of dichloromethane, approx. 1 drop of the nanofibers.
    • 1.0% 0.9899 g PLA, 10 mL of dichloromethane, approx. 1 drop of the nanofibers.
    • 5.0% 0.9488 g PLA, 10 mL of dichloromethane, approx. 1 drop of the nanofibers.
    • 10% 0.9011 g PLA, 10 mL of dichloromethane, approx. 1 drop of the nanofibers.
    • 0 % 0.9992 g PLA, 10 mL of dichloromethane, approx. 1 drop of the nanofibers.
  • The precent of the nanofibers were not right, but it was used more for labeling purposes
  • For the citrate:
    • 0.1% 0.999 g PLA, 10 mL of dichloromethane, 1 mL of citrate soln.
    • 0.5% 0.9948 g PLA, 10 mL of dichloromethane, approx. 0.8 mL of citrate
    • 1.0% 0.9894 g PLA, 10 mL of dichloromethane, approx. 0.6 mL of citrate
    • 5.0% 0.9501 g PLA, 10 mL of dichloromethane, approx. 0.4 mL of citrate
    • 10% 0.9007 g PLA, 10 mL of dichloromethane, approx. 0.2 mL of citrate


Note

The nanorfiber 0% i put into a X ray plate by adding a few drops on top.

  • The oven did not work again to flatten out the 5% MOF-5. There was a plastci thing that sat on top.