Objective
Starting of synthesis for both polymer and polymer-clay films.
Description
Perform the following procedures (1 and 2) in parallel for the start to the synthesis of cross-linked polymer and cross-linked polymer-clay films.
Note: I prepared the starting materials yesterday
- Polymer-Clay Films
- Add 7mL of water to 1g of 22,000MW polyvinyl alcohol and 0.11g of sodium montmorillonite in a glass vial
- Stir the solution with constant heating at 75C until the polymer is dissolved and the clay is dispersed (~15 minutes)
- Cool the solution to room temperature
- Add 0.5mL 0.8 wt% glutaraldehyde.
- NOTE: Perform step 4 in the hood
- Stir for an additional 3 minutes to ensure homogeneity
- Pour solution into a teflon dish to dry until the next class
- Polymer Films
- Add 7mL of water to 1g of 22,000MW polyvinyl alcohol in a glass vial
- Stir the solution with constant heating at 75C until the polymer is dissolved (~15 minutes)
- Cool the solution to room temperature
- Add 0.5mL 0.8 wt% glutaraldehyde.
- NOTE: Perform step 4 in the hood
- Stir for an additional 3 minutes to ensure homogeneity
- Pour solution into a teflon dish to dry until the next class
Data
- Add data and results here...
Notes
This area is for any observations or conclusions that you would like to note.
Use categories like tags. Change the "Course" category to the one corresponding to your course. The "Miscellaneous" tag can be used for particular experiments, as instructed by your professor. Please be sure to change or delete this tag as required so that the categories remain well organized.
|