User:Matt Hartings/Notebook/AU Biomaterials Design Lab/2014/08/27: Difference between revisions
From OpenWetWare
Line 22: | Line 22: | ||
## Stir the solution with constant heating at 75C until the polymer is dissolved and the clay is dispersed (~15 minutes) | ## Stir the solution with constant heating at 75C until the polymer is dissolved and the clay is dispersed (~15 minutes) | ||
## Cool the solution to room temperature | ## Cool the solution to room temperature | ||
## Add 0.5mL 0.8 wt% glutaraldehyde | ## Add 0.5mL 0.8 wt% glutaraldehyde. | ||
### NOTE: Perform step 4 in the hood | ### NOTE: Perform step 4 in the hood | ||
## Stir for an additional 3 minutes to ensure homogeneity | ## Stir for an additional 3 minutes to ensure homogeneity | ||
Line 30: | Line 30: | ||
## Stir the solution with constant heating at 75C until the polymer is dissolved (~15 minutes) | ## Stir the solution with constant heating at 75C until the polymer is dissolved (~15 minutes) | ||
## Cool the solution to room temperature | ## Cool the solution to room temperature | ||
## Add 0.5mL 0.8 wt% glutaraldehyde | ## Add 0.5mL 0.8 wt% glutaraldehyde. | ||
### NOTE: Perform step 4 in the hood | ### NOTE: Perform step 4 in the hood | ||
## Stir for an additional 3 minutes to ensure homogeneity | ## Stir for an additional 3 minutes to ensure homogeneity |
Revision as of 05:03, 27 August 2014
Biomaterials Design Lab | <html><img src="/images/9/94/Report.png" border="0" /></html> Main project page <html><img src="/images/c/c3/Resultset_previous.png" border="0" /></html>Previous entry<html> </html>Next entry<html><img src="/images/5/5c/Resultset_next.png" border="0" /></html> |
ObjectiveStarting of synthesis for both polymer and polymer-clay films. DescriptionPerform the following procedures (1 and 2) in parallel for the start to the synthesis of cross-linked polymer and cross-linked polymer-clay films. Note: I prepared the starting materials yesterday
Data
NotesThis area is for any observations or conclusions that you would like to note.
|