===Au:Myoglobin Nanofibers: Sample Prep for Cell Culture=== | |||
[[Image:2014_0211_myo_bsa_NPs.PNG]] | |||
*Solutions: | |||
**Au: 0.011g in 10mL to make 2.793mM solution | |||
**Myoglobin: 0.011g in 10mL to make 0.0621mM solution | |||
**TRIS dopamine: 0.038g dopamine hydrochloride and 0.024g TRIS in 20mL to make 10mM solution at pH 8.46 | |||
====Plain Scaffolds==== | |||
*4 PLA scaffolds printed for each test tube | |||
*Three test tubes filled with scaffolds and water | |||
*Autoclaved | |||
====Brute Force Nanofiber-coated Scaffolds==== | |||
*4 PLA scaffolds printed for each test tube | |||
*Gold:Myoglobin (100:1) nanofibers synthesized by above method | |||
*Nanofibers dried onto PLA scaffolds | |||
*Scaffolds submerged in water | |||
*Autoclaved | |||
====Original Method for Nanofiber-coated Scaffolds==== | |||
*4 PLA scaffolds printed for each test tube | |||
*Gold:Myoglobin (100:1) nanofibers synthesized by above procedure with scaffolds in solution | |||
*Autoclaved | |||
====Polydopamine-coated Scaffolds==== | |||
*4 PLA scaffolds printed for each test tube | |||
*Scaffolds submerged in 10mM pH 8.46 TRIS dopamine hydrochloride solution for 1 hour | |||
*Add 1mL of 0.0621 Myoglobin to each test tube, shake tube to combine, allow surface functionalization to occur for 5 hours | |||
*Rinse with deionized water and allow scaffold to dry overnight | |||
*Scaffolds submerged in water | |||
*Autoclaved | |||
====Polydopamine Nanofiber-coated Scaffolds==== | |||
*4 PLA scaffolds printed for each test tube | |||
*Scaffolds submerged in 10mM pH 8.5 TRIS dopamine hydrochloride solution for 1 hour | |||
*Add 1mL of 0.0621 Myoglobin to each test tube, shake tube to combine, allow surface functionalization to occur for 5 hours | |||
*Rinse with deionized water and allow scaffold to dry overnight | |||
*Gold:Myoglobin (100:1) nanofibers synthesized by above procedure with polydopamine-coated scaffolds in solution | |||
*Autoclaved | |||
Revision as of 16:46, 31 March 2014
Cell/Scaffold Tests | <html><img src="/images/9/94/Report.png" border="0" /></html> Main project page <html><img src="/images/c/c3/Resultset_previous.png" border="0" /></html>Previous entry<html> </html>Next entry<html><img src="/images/5/5c/Resultset_next.png" border="0" /></html> |
April 1, 2014Objectives
Au:Myoglobin Nanofibers: Sample Prep for Cell Culture
Plain Scaffolds
Brute Force Nanofiber-coated Scaffolds
Original Method for Nanofiber-coated Scaffolds
Polydopamine-coated Scaffolds
Polydopamine Nanofiber-coated Scaffolds
Type I Collagen Test (Detection and Quantification)Collagen Staining Procedure & Microscope ImagingTrypsin Cell Detachment Procedure & Cell Counting |