User:Karlena L. Brown/Notebook/PVOH Research/2013/03/08: Difference between revisions

From OpenWetWare
Jump to navigationJump to search
(fix raw html notebook nav)
 
(10 intermediate revisions by one other user not shown)
Line 2: Line 2:
|-
|-
|style="background-color: #EEE"|[[Image:owwnotebook_icon.png|128px]]<span style="font-size:22px;"> PVOH Research</span>
|style="background-color: #EEE"|[[Image:owwnotebook_icon.png|128px]]<span style="font-size:22px;"> PVOH Research</span>
|style="background-color: #F2F2F2" align="center"|<html><img src="/images/9/94/Report.png" border="0" /></html> [[{{#sub:{{FULLPAGENAME}}|0|-11}}|Main project page]]<br />{{#if:{{#lnpreventry:{{FULLPAGENAME}}}}|<html><img src="/images/c/c3/Resultset_previous.png" border="0" /></html>[[{{#lnpreventry:{{FULLPAGENAME}}}}{{!}}Previous entry]]<html>&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;</html>}}{{#if:{{#lnnextentry:{{FULLPAGENAME}}}}|[[{{#lnnextentry:{{FULLPAGENAME}}}}{{!}}Next entry]]<html><img src="/images/5/5c/Resultset_next.png" border="0" /></html>}}
|style="background-color: #F2F2F2" align="center"|[[File:Report.png|frameless|link={{#sub:{{FULLPAGENAME}}|0|-11}}]][[{{#sub:{{FULLPAGENAME}}|0|-11}}|Main project page]]<br />{{#if:{{#lnpreventry:{{FULLPAGENAME}}}}|[[File:Resultset_previous.png|frameless|link={{#lnpreventry:{{FULLPAGENAME}}}}]][[{{#lnpreventry:{{FULLPAGENAME}}}}{{!}}Previous entry]]&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;}}{{#if:{{#lnnextentry:{{FULLPAGENAME}}}}|[[{{#lnnextentry:{{FULLPAGENAME}}}}{{!}}Next entry]][[File:Resultset_next.png|frameless|link={{#lnnextentry:{{FULLPAGENAME}}}}]]}}
|-
|-
| colspan="2"|
| colspan="2"|
<!-- ##### DO NOT edit above this line unless you know what you are doing. ##### -->
<!-- ##### DO NOT edit above this line unless you know what you are doing. ##### -->
==OBJECTIVES==
==OBJECTIVES==
* Clean, filter, and separate out the oil from the previously prepared microspheres on '''2/22/13'''
==Microspheres: Separation & Vacuum Filtration Procedures==
==Microspheres: Separation & Vacuum Filtration Procedures==


==Hydrogel Pressure Samples Tested 3==
'''Setup of a vacuum filtration system:'''
'''RECALL HYDROGEL PRESSURE TESTING PROTOCOL ON 2/20/13 & FLUORESCENCE ANALYSIS PROCEDURES ON 2/13/13'''  
  * Clean 250mL Erlenmeyer Filter Flask
  * Large Buchner Funnel
  * Whatman #42 Filter Paper
  * Long Secure Rubber Hose


{| {{table}}
# Take a microsphere sample out of its container using a pair of tweezers
| align="center" style="background:#f0f0f0;"|'''Sample Order'''
# Place a piece of filter paper into the Buchner funnel, then filter the microsphere using the vacuum filtration system setup
| align="center" style="background:#f0f0f0;"|'''PVOH vs. Clay Ratio'''
# Attach all parts of the apparatus to the vacuum filtrator system
| align="center" style="background:#f0f0f0;"|'''PVOH Type'''
# Place a piece of Whatman #42 filter paper in the Buchner Funnel
| align="center" style="background:#f0f0f0;"|'''Clay Selection'''
# Turn on the vacuum filtrator system
| align="center" style="background:#f0f0f0;"|'''Amount of Hydrogel Used (g)'''
# Check the suction rate to ensure that enough pressure is applied
|-
# Place the microsphere sample into the Buchner funnel
| 1||50:50||130K||110% CEC NaMT w/ DMHXLBR||0.1006
# Allow the vacuum filtration to continue until the microsphere is completely dry
|-
# To continuously remove the oil integrated within the microsphere sample, wash the microspheres with hexanes repeatedly
| 2||50:50||130K||110% CEC NaMT w/ DMHXLBR||0.1022
# Once microspheres completely dehydrate, clean with hexanes and place microsphere samples in new small labeled vial
|-
# Allow microspheres to dry for ~ 1 day
| 3||90:10||130K||Laponite||0.1031
# Wash all glassware and equipment first with H<sub>2</sub>O and then with acetone for later use
|-
| 4||50:50||146K||110% CEC Laponite w/ DMHXLBR||0.1066
|-
| 5||90:10||130K||110% CEC Laponite w/ DMHXLBR||0.1083
|-
| 6||90:10||130K||110% CEC NaMT w/ DMHXLBR||0.1003
|-
| 7||50:50||130K||110% CEC Laponite w/ DMHXLBR||0.1036
|-
| 8||50:50||146K||Laponite||0.1016
|-
| 9||90:10||130K||110% CEC NaMT w/ DMHXLBR||0.1011
|-
| 10||90:10||146K||110% CEC NaMT w/ DMHXLBR||0.1020
|-
| 11||50:50||130K||NaMT||0.1024
|-
| 12||50:50||130K||50% CEC NaMT w/ Bu<sub>3</sub>HdP<sup>+</sup>||0.1015
|-
| 13||50:50||146K||110% CEC NaMT w/ DMHXLBR||0.0998
|-
| 14||90:10||130K||50% CEC NaMT w/ Bu<sub>3</sub>HdP<sup>+</sup>||0.1026
|}


==Notes==
==Notes==
 
* Many microsphere samples did not exactly precipitate out into smaller tiny spheres, they remained connected.
* Also many microspheres samples appeared to be very absorbent and squishy to touch
* Due to the excess amount of oil used to produce each microsphere sample, several portions and layers of oil had to be decanted off prior to rinsing extensively with hexanes -- samples were decanted by pulling off the oil using Pasteur pipettes
* For many microspheres several portions of hexanes were needed to purify, clean, and remove oil from each sample ~ 25mL (5 portions of 5mL)
<!-- ##### DO NOT edit below this line unless you know what you are doing. ##### -->
<!-- ##### DO NOT edit below this line unless you know what you are doing. ##### -->
|}
|}


__NOTOC__
__NOTOC__

Latest revision as of 22:34, 26 September 2017

PVOH Research Main project page
Previous entry      Next entry

OBJECTIVES

  • Clean, filter, and separate out the oil from the previously prepared microspheres on 2/22/13

Microspheres: Separation & Vacuum Filtration Procedures

Setup of a vacuum filtration system:

  * Clean 250mL Erlenmeyer Filter Flask
  * Large Buchner Funnel
  * Whatman #42 Filter Paper
  * Long Secure Rubber Hose
  1. Take a microsphere sample out of its container using a pair of tweezers
  2. Place a piece of filter paper into the Buchner funnel, then filter the microsphere using the vacuum filtration system setup
  3. Attach all parts of the apparatus to the vacuum filtrator system
  4. Place a piece of Whatman #42 filter paper in the Buchner Funnel
  5. Turn on the vacuum filtrator system
  6. Check the suction rate to ensure that enough pressure is applied
  7. Place the microsphere sample into the Buchner funnel
  8. Allow the vacuum filtration to continue until the microsphere is completely dry
  9. To continuously remove the oil integrated within the microsphere sample, wash the microspheres with hexanes repeatedly
  10. Once microspheres completely dehydrate, clean with hexanes and place microsphere samples in new small labeled vial
  11. Allow microspheres to dry for ~ 1 day
  12. Wash all glassware and equipment first with H2O and then with acetone for later use

Notes

  • Many microsphere samples did not exactly precipitate out into smaller tiny spheres, they remained connected.
  • Also many microspheres samples appeared to be very absorbent and squishy to touch
  • Due to the excess amount of oil used to produce each microsphere sample, several portions and layers of oil had to be decanted off prior to rinsing extensively with hexanes -- samples were decanted by pulling off the oil using Pasteur pipettes
  • For many microspheres several portions of hexanes were needed to purify, clean, and remove oil from each sample ~ 25mL (5 portions of 5mL)