(New page: =How to Create a PDMS-Stamp from Silicone/Araldite Mold= ==Preparation of PDMS mixture== * with pipette boy and 5ml stripette pour ~4g of elastomer into a cup * with micropipette (1000µl...)
 
Line 18: Line 18:
==Final Processing==
==Final Processing==
* punch holes with 2mm coring tool at the desired connection points under dissection microscope (tip: target the hole with coring tool under microscope, then put the stamp onto one finger with alufoil between stamp and finger and push/turn until you feel the coring tool on your skin)
* punch holes with 2mm coring tool at the desired connection points under dissection microscope (tip: target the hole with coring tool under microscope, then put the stamp onto one finger with alufoil between stamp and finger and push/turn until you feel the coring tool on your skin)
* [[Christian Niederauer/Notebook/RacingBacteria/Protocols/Plasma_Cleaning | plasma Clean]] the treated face of the stamp and a coverslip and press them together with alufoil in order to prevent contamination
* [[Christian Niederauer/Notebook/RacingBacteria/Protocols/Plasma_Cleaning | plasma clean]] the treated face of the stamp and a coverslip and press them together with alufoil in order to prevent contamination




Line 24: Line 24:
'''BEFORE PUNCHING HOLES'''
'''BEFORE PUNCHING HOLES'''
* take a slice of PDMS with bigger or same area than the stamp
* take a slice of PDMS with bigger or same area than the stamp
* [[Christian Niederauer/Notebook/RacingBacteria/Protocols/Plasma_Cleaning | plasma Clean]] unshaped face of stamp and extra slice and stick them together
* [[Christian Niederauer/Notebook/RacingBacteria/Protocols/Plasma_Cleaning | plasma clean]] unshaped face of stamp and extra slice and stick them together
* now punch desired holes with 2mm coring tool
* now punch desired holes with 2mm coring tool

Revision as of 07:42, 23 August 2014

How to Create a PDMS-Stamp from Silicone/Araldite Mold

Preparation of PDMS mixture

  • with pipette boy and 5ml stripette pour ~4g of elastomer into a cup
  • with micropipette (1000µl) add one tenth of elastomer mass (~0.4g) of linker fluid to the cup
  • mix well with stripette
  • degass for 30min-60min

Preparation of PDMS membrane

  • pour degassed mixture onto wafer placed in petri dish with aluminium foil
  • pour just enough to cover the waver
  • use Leveling Petri Dish to ensure constant thickness
  • araldite wafer: cure it for 3-4 hours in oven at 60°C
  • silicon wafer: cure it for 2 hours in oven at 80°C for
  • peel off membrane from wafer surface with forceps
  • cut out the pattern but leave enough space around it

Final Processing

  • punch holes with 2mm coring tool at the desired connection points under dissection microscope (tip: target the hole with coring tool under microscope, then put the stamp onto one finger with alufoil between stamp and finger and push/turn until you feel the coring tool on your skin)
  • plasma clean the treated face of the stamp and a coverslip and press them together with alufoil in order to prevent contamination


If the stamp is too thin

BEFORE PUNCHING HOLES

  • take a slice of PDMS with bigger or same area than the stamp
  • plasma clean unshaped face of stamp and extra slice and stick them together
  • now punch desired holes with 2mm coring tool